Blasting abrasives supplier
+90 216 706 70 72+90 532 063 81 58info@anadolukumlama.com

Technical Information

Surface Inspection After Blasting: Soluble Salt Test, Dust, Profile

Checks made after blasting and before painting: Sa grade, soluble salt and dust tests, surface profile measurement, dew point and why clean abrasive matters.

Published: · 5 min read

Clean garnet abrasive used in surface preparation before painting

When blasting is finished the surface may look clean, but for a long-lasting coating the things you cannot see also matter: soluble salts, fine dust and surface temperature. In this article we explain surface inspection after blasting: what is checked on the surface before painting, and how. It covers the cleanliness grade, the soluble salt test, the dust tape test, surface profile, dew point and the cleanliness of the abrasive itself.

Why is inspection needed?

Most paint and coating systems require the surface to meet certain conditions immediately before application. These conditions are written in the paint manufacturer's technical data sheet and in the job specification. Paint applied without these checks may look fine at first glance; however, blistering, underfilm rusting or early detachment appears months later, and at that point repair is very expensive.

1. Cleanliness grade (Sa)

The first check is visual. The surface is compared with the reference photographs in ISO 8501-1 to see whether the required cleanliness grade (usually Sa 2½) has been reached. Edges, corners, weld seams and shadowed areas are checked in particular. We explained the grades in our article Sa 2, Sa 2½ and Sa 3.

2. Soluble salt test (Bresle)

On steel surfaces that have been in service by the sea, in a salty environment or exposed to chemicals, invisible soluble salts (especially chlorides) can remain on the surface even after blasting. Under the paint these salts draw in moisture and lead to blistering and underfilm corrosion.

The amount of salt is commonly measured with the Bresle method: an adhesive patch is stuck to the surface, pure water is injected with a syringe to wash the surface, the water is drawn back and its conductivity is measured (ISO 8502-6 and ISO 8502-9). The result is given as the amount of salt per square metre.

  • The permitted upper limit is set by the coating system and the specification; this limit varies with the service environment and the type of coating.
  • If the limit is exceeded, the surface is usually washed with clean water, dried and, if necessary, blasted again.
Angular brown fused alumina used for blasting before painting
Angular abrasive cleans the surface and creates the roughness the paint will grip.

3. Dust test (tape test)

Blasting leaves fine dust on the surface. This dust acts as a separating layer between the paint and the steel and weakens adhesion. The amount of dust is assessed with the dust tape test according to ISO 8502-3: transparent tape is applied to the surface and pressed down, then lifted, and the quantity and particle size of the dust on the tape are compared with a reference chart. Dust is usually removed from the surface with clean, oil-free compressed air or by vacuum.

4. Roughness (surface profile)

For the paint to adhere, the surface needs a certain roughness. Too low a profile weakens adhesion; with too high a profile, the peaks can protrude through the paint film. The surface profile is measured according to the ISO 8503 series with a comparator, replica tape or a stylus profile gauge. We explained the methods in our article how to measure surface roughness.

5. Ambient conditions and dew point

Blasted steel can quickly rust again in humid air. Before painting starts, air temperature, relative humidity and surface temperature are measured. The common rule is that the surface temperature must be at least 3 °C above the dew point (ISO 8502-4). Otherwise an invisible film of moisture can form on the surface. For the concept of dew point, see the Wikipedia article on dew point.

The time between blasting and painting also matters: the surface must be painted before visible re-rusting (flash rust) begins. The acceptable time is set by the ambient conditions and the specification.

Why does abrasive cleanliness matter?

Salt on the surface does not always come from the old surface; contaminated abrasive can also carry salt and dust onto it. That is why water-soluble contaminants in abrasives are measured with the ISO 11127-6 (conductivity) and ISO 11127-7 (chloride) methods.

  • New abrasive: Ask the supplier for the product's technical data sheet and, if needed, its conductivity or chloride values.
  • Recycled abrasive: It can build up dust and dirt with every cycle. The dust separator and screen must work properly, and the abrasive should be renewed at set intervals. Details are in our article on abrasive recycling.
  • Storage: Keep the abrasive in its packaging in a dry, covered place; abrasive that gets wet or damp does not flow and carries moisture onto the surface.
Clean steel grit used in recycling blast cabinets
In recycling systems, the dust separator must work properly for the steel grit to stay clean.

Frequently asked questions

How soon after blasting should painting be done?

As soon as possible, and in any case before visible re-rusting begins. The accepted time depends on the humidity and temperature of the environment, the specification and the coating system.

Is a salt test required on every job?

It is not mandatory on every job; the specification decides. It is usually required on surfaces with a high salt risk, such as marine structures, ships, tanks and steel working in chemical environments.

How is dust removed from the surface?

After blasting, the surface is usually blown down with clean, dry, oil-free compressed air or vacuum cleaned. The result is checked with the tape test. Touching the surface with bare hands is not recommended, as it can leave oil and salt.

Request a quote for clean abrasive

Tell us your blasting system, the surface and the cleanliness and profile values in your specification in the quote form, and we will choose the right abrasive together. You can browse all products, including garnet, brown fused alumina and steel grit, on our products page.

Which material and grain size suit your job?